Why specify ASTM A194 Grade 2HM instead of 2H?

Grade 2H has the higher proof-load requirement. Grade 2HM has the lower maximum hardness, which matters when the bolting is exposed to wet hydrogen sulfide.

November 25, 2026HexFastener

The short answer. Specify 2HM when the joint calls for a hardness-controlled carbon steel nut. In wet hydrogen sulfide service, limiting hardness helps reduce the risk of sulfide stress cracking. The change also lowers the nut’s required proof load. [1] [3]

This article in the ASTM A194 series looks at the choice on a control valve bonnet.

On a Fisher ES control valve with a WCC carbon-steel body, the standard bonnet fasteners for sour service are B7 studs with 2H nuts where the bolting is unexposed. Fisher offers B7M studs with 2HM nuts for exposed bolting on that same valve. A request for “bonnet nuts for sour service” could therefore bring back two different quotes.[2]

What the nut threads have to carry

A ¾–10 heavy hex 2HM nut fits the same stud as a 2H of that size. In the proof test, each screws onto a hardened steel mandrel that loads the nut along its axis. At this size, the specified test load is 8,350 lbf higher for the 2H nut.[1]

Finished ¾–10 UNC heavy hex nuts under ASTM A194/A194M-24, Tables 2 and 3
GradeProof load (lbf)Brinell hardness (HBW)
143,420121 minimum
250,100159–352
2H58,450248–327
2HM50,100159–235

Grades 2 and 2HM share the 50,100 lbf proof load. A Grade 2 nut measuring 300 HBW is within its hardness range. At the same reading, a 2HM nut exceeds its 235 HBW ceiling, even if its threads hold.[1]

Why put a ceiling on hardness?

Water containing hydrogen sulfide can corrode steel and allow hydrogen to enter it. Under tensile stress, a susceptible steel can then crack. This is sulfide stress cracking. Harder regions of carbon steel are generally more susceptible. A nut can pass a proof test on a mandrel and still be vulnerable to cracking once the joint is in service.[3] [4]

The nut maker can produce 2H and 2HM from the same heat of carbon steel. Both grades are liquid quenched. The 2024 specification then calls for tempering at a minimum of 850°F for 2H and 1,150°F for 2HM. For 2HM, a final temper after machining, cutting and forming can also serve as the required stress relief. The hardness limit applies to each finished 2HM nut, and each one is tested.[1]

Can an external bonnet nut count as exposed?

Yes. Consider a bonnet whose nuts sit outside the flow passage but underneath insulation. For oil and gas production equipment covered by ISO 15156-2, the rules for sour-service bolting expressly include that installation, as well as buried bolting and bolting fitted with flange protectors. The standard lists ASTM A194 Grade 2HM among the acceptable nut materials.[5]

On the Fisher ES, choosing the exposed-bolting option can affect the rating of the assembled valve. Fisher retains the Class 300 rating with B7M studs and 2HM nuts. For a Class 600 valve it directs the user to Fisher to determine whether the pressure rating must be reduced.[2]

For replacement parts, use the exposure classification and bolting combination on the valve specification. If it calls for Fisher’s exposed option, put SA-193 Grade B7M studs and SA-194 Grade 2HM nuts on the order, along with the thread, nut style and specification editions called for by the project. For alloy and stainless grades on other drawings, see the ASTM A194 grade index.

For alloy steel nuts with a hardness limit or an impact-test requirement, continue with A194 Grades 7 and 7M.

References

  1. ASTM A194/A194M-24, Tables 1–3, pp. 3–6, and §§6.3–6.5 and 8.1–8.2. Chemistry, heat treatment, finished-nut hardness and inch-series proof loads.
  2. Emerson, Fisher ES and EAS Sliding-Stem Control Valves, bulletin D100021X012, October 2025, p. 17, Table 11 and note 2. Fisher uses the ASME SA-193 and SA-194 designations for this valve.
  3. AMPP, Corrosion Terminology, entry for sulfide stress cracking.
  4. TWI, The Effect of Low H₂S Concentrations on Welded Steels, March 2000. Influence of hardness, stress and hydrogen on cracking susceptibility.
  5. ISO 15156-2:2020, Annex A, §A.2.2.4 and Table A.4. Bolting exposure and acceptable materials for oil and gas production equipment.