The short answer. A cold-service flange exposed to wet hydrogen sulfide may call for ASTM A320 L7M because limiting stud hardness helps control susceptibility to sulfide stress cracking. L7M specifies 200–235 HBW. For a ¾-in. stud, changing from L7 to L7M lowers the minimum yield strength from 105 to 80 ksi and changes the standard impact test temperature from −150 to −100 °F. A320 calls for a Grade 7M mating nut. [1]

This part of the ASTM A320 bolting series covers the choice where cold service and exposure to wet hydrogen sulfide occur in the same joint.

The two studs can be made from the same chromium-molybdenum steel. For a replacement on a gas-production flange, the following differences matter even when the new stud threads straight into the old nut. [1] [2]

¾-in. studs, inch-series requirements in ASTM A320/A320M-26. Strength values are room-temperature minimums.
RequirementL7L7M
Tensile / yield strength125 / 105 ksi100 / 80 ksi
Brinell hardness321 HBW maximum200–235 HBW
Minimum tempering temperature1,100 °F1,150 °F
Charpy test temperature, standard order−150 °F−100 °F

Why a harder stud can be the wrong choice

Where steel under tension encounters water containing hydrogen sulfide, hydrogen can enter the steel and contribute to sulfide stress cracking. Hardness is one of the factors that governs susceptibility. ISO 15156-2 lists L7M among the bolting materials for the oil and gas production environments it covers. Its rules take account of how the bolting is exposed. Insulation or flange protectors can shield an external stud from open air, so “outside the pipe” alone does not settle the question. [2]

For an L7M order the hardness window applies to each bolt or stud. A320 permits either indentation testing of every piece or qualified electromagnetic examination of every piece backed by indentation sampling. A single Brinell reading of 220 HBW is within the range. By itself, it shows neither how the rest of the lot was checked nor whether the stud met the tensile requirements. [1]

What changes at the flange

At the same thread size, a design that relies on the 105 ksi minimum yield strength of L7 needs review before substitution with 80 ksi L7M. ISO 15156-2 specifically draws attention to the possible effect of cracking-resistant bolting on equipment pressure ratings. The designer must account for the lower strength when confirming the joint rating and assembly load. [1] [2]

Carry the change through to the nuts. For this ¾-in. assembly, A320 specifies Grade 7M nuts with a maximum hardness of 235 HBW and requires impact testing of their material. A194 identifies the nut grade. The additional L marking identifies nut material that has been impact tested. [1]

A cold sour-service drawing can also ask for a test below −100 °F. For a specified −150 °F test, ask for the L7M lot results at that temperature or colder, meeting the specified energy limits, and confirm the applicable temperature marking. An L7 report for a different heat cannot establish the impact properties of those L7M studs. [1]

Where diameter is the difficulty and the design still requires 125 ksi tensile strength, the comparison shifts to ASTM A320 Grade L43 for Large-Diameter Studs.

References

  1. ASTM A320/A320M-26. Tables 1–3 and §§6.2, 6.3.2, 10.1 and 13.2. Grade properties, piece hardness examination, nuts and marking.
  2. ISO 15156-2:2020. Oil and gas production in H₂S-containing environments. See §7 and Annex A.2.2.4, including Table A.4, for material selection and bolting exposure.