American SAE J403 Low-Carbon Steel Grades: What Are 1006, 1018 and 1022?

SAE 1006, 1008, 1010, 1015, 1018, 1020 and 1022 steel: carbon and manganese ranges, cold-heading choices and the role of delivery condition.

November 15, 2026HexFastener

The short answer: SAE 1006–1022 are low-carbon steel grades whose carbon and manganese limits help determine forming behavior and the available heat-treatment routes.

A rivet blank with a large upset and a case-hardened screw can both start with low-carbon stock, yet put different demands on it. The rivet needs enough ductility for forming; the screw’s chemistry must also suit its specified surface-hardening route. Carbon, manganese and the supplied condition help narrow the choice.

The SAE 1006–1026 grade family

In the familiar SAE four-digit system, 10xx identifies a plain-carbon steel family. The final two digits indicate an approximate nominal carbon level in hundredths of a percent. The actual limits come from the grade table: 1018 contains 0.15–0.20% C in the source below, while 1020 contains 0.18–0.23% C. The number is a designation, rather than a batch analysis. [1] [2]

SAE J403_202402 defines carbon-steel chemistry. You will also encounter the established names “AISI 1018” and “AISI 1020”; SAE now maintains these designations. For cold-headed fasteners, the order also needs the appropriate rod or wire quality and delivery condition. [3] [4]

Carbon and manganese: the actual ranges

The selected grades below show both the low-carbon end and the neighboring 1025/1026 grades. All compositions are percentages by mass. A maximum such as ≤0.08% gives an upper limit; a range such as 0.08–0.13% gives both limits.

GradeC (%)Mn (%)P max. (%)S max. (%)
1006≤0.080.25–0.400.0300.050
1008≤0.100.30–0.500.0300.050
10100.08–0.130.30–0.600.0300.050
10120.10–0.150.30–0.600.0300.050
10150.13–0.180.30–0.600.0300.050
10170.15–0.200.30–0.600.0300.050
10180.15–0.200.60–0.900.0300.050
10200.18–0.230.30–0.600.0300.050
10210.18–0.230.60–0.900.0300.050
10220.18–0.230.70–1.000.0300.050
10250.22–0.280.30–0.600.0300.050
10260.22–0.280.60–0.900.0300.050

Heat analysis, mass percent; selected elements, not a complete purchase specification. Selected producer-handbook rows labeled SAE J403-24. Lower P/S limits and silicon practice may be specified for particular cold-heading orders. [2]

Silicon limits and deoxidation practice can vary with the order. Where they affect the forming route, agree them with the supplier; the cited table allows several specified silicon ranges for these steels. [2]

What each group is useful for

1006 and 1008: leave room for deformation

The lowest-carbon rows are starting points when the head or body needs substantial cold deformation. Rivets, lightly loaded formed parts and simple screws can benefit from a low-carbon substrate. Low carbon limits the hardness available from conventional quenching, so choose the finished-part requirement before selecting the stock. [5]

1010, 1012 and 1015: add carbon gradually

These grades move the carbon interval upward without introducing a chromium or molybdenum alloy design. They provide intermediate choices where the manufacturer needs a balance between forming load and the properties developed by cold working or a specified surface-hardening process. Annealed wire and heavily drawn wire of one grade can behave quite differently. [5]

1017 and 1018: same carbon, different manganese

Both rows contain 0.15–0.20% C, but 1018 has 0.60–0.90% Mn against 1017’s 0.30–0.60%. Manganese increases hardenability and contributes to strength. The practical choice therefore depends on more than the last two digits. [2] [6]

1020, 1021 and 1022: compare manganese at fixed carbon

These three grades share 0.18–0.23% C in this table. Their Mn intervals are 0.30–0.60%, 0.60–0.90% and 0.70–1.00%, respectively. 1022 offers a higher-manganese chemistry within the same carbon window; it is useful to consider when both forming and a subsequent hardening operation matter. [2]

The following plot makes these overlapping intervals easier to compare.

1018 and 1020 have overlapping carbon ranges but different manganese ranges. 1020, 1021 and 1022 share the listed carbon interval. Range bars show chemistry limits, not measured strengths.
1018 and 1020 have overlapping carbon ranges but different manganese ranges. 1020, 1021 and 1022 share the listed carbon interval. Range bars show chemistry limits, not measured strengths. [2]

1018 versus 1020: what changes in the part?

1018 has less nominal carbon than 1020, but more manganese in the listed specification. The carbon ranges overlap, so a particular 1018 heat can have more carbon than a particular 1020 heat. Compare the actual certificate and the supplied condition when the difference matters. The series guide explains heat versus product analysis when checking a reported composition against these limits. [2]

Cold drawing can raise strength while reducing the deformation remaining for heading. Annealing prepares the stock for further forming. Carburizing raises carbon near the surface, allowing a hard case with a lower-carbon core after the specified hardening treatment. These routes answer different part requirements; none gives one universal “1018 tensile strength.” [5]

When to move beyond low-carbon 10xx

If the part needs more hardness throughout its section, consider the 1035–1050 carbon steels. If the limiting issue is hardening deeper into a section while keeping carbon relatively low, compare higher-manganese 15xx grades or boron-treated grades such as 10B21. Those changes serve different purposes.

For a cold-heading order, specify the SAE grade, wire or rod diameter, delivery condition, surface requirements and applicable ASTM F2282 quality requirements. State the finished screw or bolt specification separately so the processor can select and verify the forming and heat-treatment route. [4]

References

  1. SAE J402_202403 — New Steel Designation System for Wrought or Rolled Steel (stabilized March 2024)
  2. China Steel Corporation, Bar & Wire Rods Product Manual (2025), §§6.1.2, 6.1.16–6.1.18, pp. 13, 23–25
  3. SAE J403_202402 — Chemical Compositions of SAE Carbon Steels (stabilized February 2024)
  4. ASTM F2282-23 — Quality Assurance Requirements for Carbon and Alloy Steel Wire, Rods, and Bars for Mechanical Fasteners
  5. Metallus, Practical Data for Metallurgists, 19th edition (2024), pp. 4–7 and glossary
  6. Nippon Steel, Special Steel Strip, U112en, section on the effects of alloying elements