Engineering Guide · 3 min read
Cold Heading with Boron Steel: SAE 10B21, 10B22 and 10B38 (J403)
What boron does in 10B21, 10B22, 10B33 and 10B38: published producer chemistry, B in ppm, active boron and the choice between forming and hardening.
The short answer: Boron-treated carbon steels use a very small effective boron addition to improve hardenability, allowing lower-carbon grades to combine cold forming with subsequent hardening.
A deep head recess or a substantial cold upset puts a premium on deformable incoming wire. If the finished part also needs hardening, a lower-carbon boron grade can help the manufacturer meet both demands within a suitable heat-treatment route.
What B means in 10B21
The inserted B identifies a boron addition in the SAE designation system. 10B21 and 10B22 sit in the low-carbon boron group; 10B33 and 10B38 carry more carbon. Boron acts mainly on the steel’s transformation behavior during cooling, helping martensite form farther into the section under an appropriate hardening treatment. [1] [2]
That distinguishes the approach from simply moving to 1045 or 1050. Carbon strongly affects the attainable hardened condition; effective boron mainly helps the section reach that condition at the available cooling rate.
10B21, 10B22, 10B33 and 10B38: published compositions
The table below uses one identified producer’s specifications so the complete set of selected limits stays together. CSC labels these rows as its own boron-steel specifications. A purchase order should identify that specification or agree its own complete limits; the bare grade name alone is less precise.
| Producer grade | C (%) | Mn (%) | Si (%) | B (%) |
|---|---|---|---|---|
| 10B20 | 0.18–0.23 | 0.30–0.60 | ≤0.10 | ≥0.0005 |
| 10B21 | 0.18–0.23 | 0.70–1.00 | ≤0.10 | ≥0.0005 |
| 10B22 | 0.18–0.23 | 0.70–1.00 | ≤0.10 | ≥0.0005 |
| 10B29 | 0.26–0.30 | 0.70–1.00 | 0.15–0.35 | ≥0.0005 |
| 10B33 | 0.32–0.36 | 0.70–1.00 | 0.15–0.35 | ≥0.0005 |
| 10B38 | 0.35–0.42 | 0.70–1.00 | 0.15–0.35 | ≥0.0005 |
Heat analysis, mass percent; selected elements, not a complete purchase specification. These six rows are explicitly CSC producer specifications, rather than universal SAE J403 chemistry rows. P and S are each ≤0.025%. The listed B value is a minimum; it is not an open-ended processing recommendation. Agree a complete B range and hardenability requirement with the supplier. [3]
In this producer table, 10B21 and 10B22 have identical limits for the elements displayed. The next material change is clearer in 10B29, 10B33 and 10B38, where carbon rises. To choose between 10B21 and 10B22 products, compare the supplier’s complete specification, delivered condition and hardenability results. [3]
How small is the boron addition?
One percent equals 10,000 parts per million by mass. Therefore 0.0005% B = 5 ppm, and 0.0030% B = 30 ppm. CSC’s separate note on boron-treated, fine-grain carbon steels describes 0.0005–0.0030% B. Its proprietary rows above state only a minimum of 0.0005%; those two specifications retain their different meanings. [3]
The figure separates the carbon intervals from the boron-scale conversion.
Why titanium and nitrogen matter
The useful boron must remain effective in the steel. If boron combines with nitrogen as boron nitride, less remains available to produce the intended hardenability effect. Titanium can bind nitrogen first, helping preserve effective boron. Steelmaking practice and the subsequent thermal cycle therefore matter alongside the reported total B content. [2]
The producer table does not specify titanium for every listed grade. If the order needs limits for Ti, N, Al or effective boron, agree them explicitly with the mill. For a demanding hardening operation, obtain the required hardenability results as well as the chemistry certificate.
The gain in forming, and the limit in tempering
A lower-carbon boron grade can reduce the forming burden compared with a higher-carbon steel chosen to achieve a similar finished requirement. Some boron substitutions need a lower tempering temperature to retain the target hardness than the alloy steel they replace. Check the finished-fastener specification’s minimum tempering requirement and the part’s service-temperature requirements before approving that route. [2]
For a thick section or a requirement that favors a different tempering response, compare 4037 and CrMo steels. Specify the permitted raw-material chemistry, hardenability requirement, section size and final mechanical properties together. A successful boron-steel choice balances the blank’s formability with the heat-treated part’s required condition.